I'm printing xmas gifts. In pic related there's a lamp.
I'm printing with:
>Ender 3 pro
>Sunlu PLA white (I'm not liking it)
>213°C
>50°C for raft and first layer, then I turn off the bed

I'm experiencing lots of stringing and, as you can see, the interior of the print is quite a mess. Cleaning is hard and tirious because the blobs are really well attached.

Any clue where I can start to try to solve the problem?
I would try to decriese the nozzle to 200.